YIN Jia-min1, WU Zhan-song21.Guangdong Electric Power Design Institute. CORROSION CHARACTERS OF TP347H STEEL UNDER ATMOSPHERE OF SUPERHEATERS OF BIOMASSBURNED BOILERS(Ⅱ)[J]. Thermal power generation, 2009, 38(8): 41-45.
YIN Jia-min1, WU Zhan-song21.Guangdong Electric Power Design Institute. CORROSION CHARACTERS OF TP347H STEEL UNDER ATMOSPHERE OF SUPERHEATERS OF BIOMASSBURNED BOILERS(Ⅱ)[J]. Thermal power generation, 2009, 38(8): 41-45.DOI:
TP347H在生物质锅炉过热器气相条件下的腐蚀特性
摘要
模拟生物质锅炉过热器区的气相条件以及过热器管壁沾灰状况
在500~600℃范围内对奥氏体不锈钢TP347H进行了腐蚀试验研究。通过测定试样的增重量
得出了腐蚀动力学曲线;利用配有能谱分析仪的扫描电镜和X射线衍射仪
对试样腐蚀后的形貌结构、元素含量和腐蚀产物的组成成分进行了分析。结果表明
当试片表面存在生物质灰时
TP347H的腐蚀速率比无灰大大增加;沾有生物质灰的TP347H对反应温度非常敏感
随着反应温度的增加
TP347H的抗腐蚀性能逐渐降低。
Abstract
A study on corrosion test of TP347H austenic stainless steel has been carried out in a temperature range of 500~600 ℃
simulating the atmosphere and ash deposition on tube-wall of superheaters in biomass-burned boilers.The corrosion dynamic curves have been obtained through mass gain;the appearance
elements content
and composition of corrosion products after corrosion of specimens being analysed by using the scanning electron microscope(SEM) equiped with energy dispersive spectrometer(EDS) and X-ray diffraction(XRD) meter.Test shows that the corrosion rate of TP347H steel with biomass ash deposition is greatly increased compared with that without biomass ash deposition;the TP347H steel with biomass ash deposition is very sensitive to the reaction temperature
the anti-corrosion performance of TP347H steel is gradually decreased with the increase of reaction temperation.