STUDY ON PURE OCTADECYLAMINE FILM-FOMING CHARACTERS OVER METALLIC MATERIALS COMMONLY USED FOR THERMAL POWER UNITS UNDER HIGH-TEMPERATURE CONDITION
|更新时间:2025-09-28
|
STUDY ON PURE OCTADECYLAMINE FILM-FOMING CHARACTERS OVER METALLIC MATERIALS COMMONLY USED FOR THERMAL POWER UNITS UNDER HIGH-TEMPERATURE CONDITION
Thermal Power GenerationVol. 40, Issue 12, Pages: 30-33(2011)
作者机构:
1. 华东电力设计院
2. 苏州热工研究院有限公司
3. 武汉大学动力与机械学院
作者简介:
基金信息:
DOI:
CLC:TM621.8
Published:2011
稿件说明:
移动端阅览
WANG Lu1, XIE Jianli2, HU Jiayuan3 1.East China Electric Power Design Institute. STUDY ON PURE OCTADECYLAMINE FILM-FOMING CHARACTERS OVER METALLIC MATERIALS COMMONLY USED FOR THERMAL POWER UNITS UNDER HIGH-TEMPERATURE CONDITION[J]. Thermal power generation, 2011, 40(12): 30-33.
DOI:
WANG Lu1, XIE Jianli2, HU Jiayuan3 1.East China Electric Power Design Institute. STUDY ON PURE OCTADECYLAMINE FILM-FOMING CHARACTERS OVER METALLIC MATERIALS COMMONLY USED FOR THERMAL POWER UNITS UNDER HIGH-TEMPERATURE CONDITION[J]. Thermal power generation, 2011, 40(12): 30-33.DOI:
STUDY ON PURE OCTADECYLAMINE FILM-FOMING CHARACTERS OVER METALLIC MATERIALS COMMONLY USED FOR THERMAL POWER UNITS UNDER HIGH-TEMPERATURE CONDITION
摘要
采用GCF型高压釜模拟高于350℃下的水汽环境
对20G、T22、SA210A-1等3种火电机组水汽系统常用材质进行了十八胺成膜试验
依据硫酸铜点滴试验、交流阻抗、极化曲线等方法评价成膜效果
并利用Matlab 6.5对结果进行回归分析。结果表明:在温度为470~490℃
十八胺浓度为60~70mg/L
恒温时间为3~5h
pH值为8.8左右时
3种金属材料表面均能形成很好的保护膜
其中pH值对成膜效果影响最大
最佳pH值为9.0。此外
十八胺在不同金属表面成膜效果存在差异。
Abstract
By using GCF type high-pressure cauldron to simulate the water-steam environment higher than 350 ℃
the film-forming test of three kinds of metals commonly used in water-steam systems of thermal power units
namely 20G
T22
and SA210A-1
has been carried out by using pure octadecylamine under water-steam environment of temperature higher than 350 ℃
and the effectiveness of film-forming being evaluated by using methods of copper sulfate spot out test
ac resistance
and the polarization curve.The regression analysis of film-forming results has been carried out using software MATLAB 6.5.Results show that the very good film can form on surface of three said metallic materials under temperature 470~490 ℃
and the concentration of octadecy lamine being 60~70 mg/L
the time of constant temperature being 3~5 h
and the pH value being about 8.8
among these factors
the influence of pH value upon film-forming effectiveness is the largest
the optimal pH value is 9.0.The film-forming effectiveness of octadecylamine on surface of different metallic materials boasts difference.